Table 1 Sample composition, crystallite size, BET a total pore volume of prepared samples

From: TiO2-graphene oxide nanocomposite as advanced photocatalytic materials

Sample

Graphene oxide [g]

Crystallite size [nm]

Cell parameter a [Å]

Cell parameter c [Å]

BET [m2g-1]

Total pore volume [ cm3g-1]

TiGO_001

0.005

49.6

3.7963(2)

9.5144(5)

100..2

0.6530

TiGO_005

0.001

51.9

3.7968(4)

9.5121(4)

151.4

0.7846

TiGO_010

0.01

52.2

3.7970(2)

9.5121(6)

195.7

1.4668

TiGO_050

0.05

34.5

3.7970(3)

9.5086(8)

185.7

0.623

TiGO_075

0.075

34.5

3.7973(2)

9.5077(7)

119.2

0.6501

TiGO_100

0.100

32.1

3.7973(6)

9.5060(4)

168.4

0.6687

TiGO_200

0.200

35.0

3.7971(4)

9.5047(5)

178.0

0.6247

TiGO_300

0.300

46.7

3.7954(5)

9.5118(7)

78.9

0.618

TiGO_400

0.400

43.6

3.7954(2)

9.5106(6)

68.6

0.5545

TiGO_500

0.500

39.1

3.7955(6)

9.5095(8)

78.1

0.6089