Time (hours)

Conv. (%)a

M n b

PDIb

P r c

Ti(1)(OiPr)2

24

54

12050

1.07

0.56

Ti(2)(OiPr)2

24

50

7900

1.19

0.63

Ti(3)(OiPr)2

24

42

7050

1.14

0.53

Ti(4)(OiPr)2

24

41

6750

1.10

0.63

Ti(5)(OiPr)2

24

60

10900

1.14

0.61

Ti(6)(OiPr)2

24

51

6850

1.23

0.55