Skip to main content

Table 2 Structural information obtained from XRD patterns of collagen fibrils after IPA treatment, rehydration and air-drying

From: Effects of isopropanol on collagen fibrils in new parchment

IPA %

intermolecular lateral packing nm

(sd)

axial D-periodicity nm

(sd)

helical rise per residue nm

(sd)

0

1.212 (+/- 0.011)

62.6 (+/- 0.03)

0.286 (+/- 0.0007)

10

1.197(+/- < 0.001)

62.5 (+/- 0.06)

0.286 (+/- 0.0003)

20

1.203 (+/- 0.006)

62.7(+/- 0.02)

0.286 (+/- 0.0004)

30

1.211 (+/- 0.004)

62.8 (+/- 0.03)

0.286 (+/- 0.0006)

40

1.179 (+/- 0.004)

62.6 (+/- 0.09)

0.285 (+/- 0.0004)

50

1.168 (+/- 0.004)

62.6 (< 0.07)

0.286 (+/- 0.0001)

60

1.176 (+/- 0.002)

62.5 (+/- 0.08)

0.285 (+/- 0.0005)

70

1.146 (+/- 0.002)

63.7 (+/- 0.04)

0.289 (+/- < 0.0001)

80

1.149 (+/- 0.003)

63.7 (< 0.01)

0.289 (+/- 0.0009)

90

1.151 (+/- 0.004)

64.0 (+/- 0.05)

0.289 (+/- 0.0004)

100

1.132 (+/- 0.007)

64.1 (+/- 0.03)

0.290 (+/- 0.0002)