Table 1 Surface area, total pore volume, crystallite size and phase composition of Sn 4+ series of TiO 2

From: Hydrogen peroxide route to Sn-doped titania photocatalysts

Sample

SnCl4 [ml]

Sn [wt.%]

Surface Area [m2g-1]

Total Pore Volume [cm3g-1]

Anatase by XRD [%]

Anatase Cryst. Size [nm]

Rutile by RD [%]

Rutile Cryst. Size [nm]

Brookite by XRD [%]

Brookite Cryst. Size [nm]

TiSn401

0.1

0.71

96.5

0.32

84.1

46.2

11.2

43.3

4.7

30.1

TiSn403

0.3

1.03

101.5

0.33

75.5

47.8

18.5

25.7

6.0

47.0

TiSn405

0.5

1.97

121.1

0.27

65.5

49.2

19.3

18.9

15.2

36.7

TiSn407

0.7

3.45

140.0

0.32

46.1

32.5

50.4

16.1

3.5

34.4

TiSn410

1.0

5.04

157.7

0.23

5.1

-

88.5

15.9

6.4

24.3

TiSn420

2.0

9.30

194.6

0.20

-

-

100

15.6

-

-

TiSn430

3.0

12.27

185.9

0.21

-

-

100

10.2

-

-